- Chemical resistance

High
volume paper handling systems require a roller with high abrasion
resistance and consistent coefficient of friction for long part life
and jam-free operation. These rollers were formulated from solid Durethane
S, a solid elastomer capable of excellent heat dissipation and wear
in paper handling and transport applications.
The table represents typical
ranges of physical properties for materials formulated from Durethane S.
For information about custom formulation and the specific values attainable
for your application, please call our sales department at +1 (401) 946-4400.
|
MPC, DURETHANE S
SHORE A
|
|
NAME
|
HARDNESS
|
BACKBONE
|
BACKBONE
|
TENSILE MODULUS
|
ELONGATION
|
TEAR STRENGTH
|
COMPRESSION
|
|
Shore A
|
TDI
|
MDI
|
AT 100% (PSI) 2
|
%
|
DIE-C (PLI)
|
SET %
|
| DS-210A |
10A
|
ESTER
|
|
35
|
575
|
45
|
3
|
| DS-715A |
15A
|
|
ETHER
|
50
|
450
|
25
|
4
|
| DS-720A |
20A
|
|
ETHER
|
55
|
420
|
30
|
5
|
| DS-220A |
20A
|
ESTER
|
|
50
|
550
|
55
|
4
|
| DS-230A |
30A
|
ESTER
|
|
95
|
650
|
90
|
5
|
| DS-330A |
30A
|
ETHER
|
|
80
|
1100
|
85
|
5
|
| DS-240A |
40A
|
ESTER
|
|
135
|
950
|
95
|
5
|
| DS-340A |
40A
|
ETHER
|
|
110
|
990
|
90
|
7
|
| DS-245A |
45A
|
ESTER
|
|
175
|
870
|
145
|
7
|
| DS-250A |
50A
|
ESTER
|
|
215
|
850
|
175
|
8
|
| DS-350A |
50A
|
ETHER
|
|
215
|
320
|
95
|
15
|
| DS-260A |
60A
|
ESTER
|
|
275
|
920
|
200
|
13
|
| DS-360A |
60A
|
ETHER
|
|
290
|
725
|
235
|
17
|
| DS-660A |
60A
|
|
ESTER
|
200
|
650
|
390
|
10
|
| DS-265A |
65A
|
ESTER
|
|
360
|
960
|
260
|
15
|
| DS-270A |
70A
|
ESTER
|
|
430
|
955
|
300
|
19
|
| DS-370A |
70A
|
ETHER
|
|
350
|
850
|
350
|
17
|
| DS-670A |
70A
|
|
ESTER
|
470
|
530
|
420
|
24
|
| DS-280A |
80A
|
ESTER
|
|
600
|
800
|
400
|
20
|
| DS-380A |
80A
|
ETHER
|
|
690
|
550
|
425
|
25
|
| DS-680A |
80A
|
|
ESTER
|
630
|
575
|
345
|
27
|
| DS-285A |
85A
|
ESTER
|
|
580
|
550
|
500
|
28
|
| DS-385A |
85A
|
ETHER
|
|
770
|
510
|
500
|
28
|
| DS-685A |
85A
|
|
ESTER
|
730
|
570
|
520
|
35
|
| DS-290A |
90A
|
ESTER
|
|
790
|
475
|
360
|
28
|
| DS-390A |
90A
|
ETHER
|
|
985
|
425
|
350
|
29
|
| DS-395A |
95A
|
ETHER
|
|
1665
|
350
|
345
|
29
|
| DS-695A |
95A
|
|
ESTER
|
1660
|
510
|
710
|
38
|
|
SHORE D
|
|
NAME
|
HARDNESS
|
BACKBONE
|
BACKBONE
|
TENSILE MODULUS
|
ELONGATION
|
TEAR STRENGTH
|
COMPRESSION
|
|
Shore A 1
|
TDI
|
MDI
|
AT 100% (PSI) 2
|
% 2
|
DIE-C (PLI) 3
|
SET % 4
|
| DS-545D |
45D
|
ETHER
|
|
1665
|
350
|
345
|
29
|
| DS-550D |
50D
|
ETHER
|
|
2200
|
350
|
500
|
32
|
| DS-450D |
50D
|
ESTER
|
|
1660
|
440
|
730
|
32
|
| DS-555D |
55D
|
ETHER
|
|
1645
|
350
|
390
|
33
|
| DS-560D |
60D
|
ETHER
|
|
3700
|
300
|
630
|
28
|
| DS-665D |
65D
|
|
ESTER
|
3475
|
200
|
625
|
31
|
| DS-570D |
70D
|
ETHER
|
|
4650
|
220
|
820
|
34
|
| DS-570DG |
70D
|
ETHER
|
|
5000
|
210
|
925
|
35
|
| DS-575D |
75D
|
ETHER
|
|
4770
|
220
|
1100
|
36
|
| DS-580D |
80D
|
ETHER
|
|
5650
|
240
|
920
|
45
|
| DS-580DR |
80D
|
ETHER
|
|
|
180
|
|
|
| DS-780DR |
80D
|
|
ETHER
|
|
15
|
|
|
| DS-585DR |
85D
|
ETHER
|
|
|
40
|
|
|
1
HARDNESS D2240, SHORE A, D
2 ASTM D412
3 ASTM D624, DIE-C
4 ASTM D395B @ 158F, 22 HRS